Repairing and Restoring Chipped, Pottery, China, Ceramic or Figurine

by lakesidepottery in Workshop > Repair

64371 Views, 174 Favorites, 0 Comments

Repairing and Restoring Chipped, Pottery, China, Ceramic or Figurine

01-chipped-plate-rim.jpg
How to repair broken ceramic and pottery

Cementing, filling and preparing surface for painting of chipped pottery, ceramic or china vessels.

MORE REPAIR AND RESTORATION LESSONS

BEFORE AND AFTER EXAMPLES

REPAIR COST ESTIMATE

What Will You Need - Cementing Ceramic Pieces

00-mending-what-needed.jpg

1. Two-part clear 5 minutes PC Clear epoxy (where to purchase)

2. Wooden stick, paper clip or a pin-tool

3. A container with pvc pebbles, rice or sand

4. Razor blade

5. Denatured or 91% Alcohol

6. Paper pad to mix Epoxy on

7. Good light

8. Protective eyewear

IMPORTANT: Ceramic restoration materials are not food safe, liquid or heat proof (over 190 degree F) and repaired items should not be used on cooking or food serving ware more...

Cementing Ceramic Pieces Steps

2-part-clear-epoxy.jpg
02-mix-2-part-clear-epoxy.jpg
03-apply-epoxy-piece-1.jpg
04-spread-epoxy-evenly.jpg
05-apply-first-piece.jpg
06-squeeze-piece-hard-in-pl.jpg
07-apply-next-piece.jpg
08-push-in-place.jpg
  1. Clean all surfaces and possible old glues (see how to remove old adhesive lesson)
  2. Place even amounts of 5-minutes clear epoxy (where to purchase) on a paper or cardboard pad.
  3. Mix epoxy well with a pin tool, paper clip or a wooden stick.
  4. Apply epoxy mix to one side using a pintool or a wooden stick.
  5. Use only enough adhesive to cover the edge. Too little will leave gaps, resulting in a weak repair.
  6. Place broken piece over the epoxy. Important: You have only about 60-90 seconds from start of epoxy mixing to complete the broken piece permanent placement before the epoxy becomes gummy and not workable.
  7. Quickly join the pieces together while applying light pressure to squeeze extra epoxy out. You only have about 60–90 seconds from start of epoxy mixing to placement before the epoxy becomes gummy and unworkable. Do not wipe off the squeezed off epoxy to avoid smearing.
  8. If your item is broken to more than a couple of pieces, plan the attachment sequence to avoid being left with a final piece that cannot be easily attached or fit in. Numbering the pieces after a dry run is a good idea and will assist in the actual implementation.
  9. Verify that pieces can stay steady during the cure period (let it cure at 75 degrees F or warmer).

Cementing Subsequent Pieces

09-dry-run-next-piece.jpg
10-apply-epoxy.jpg
11-spread-epoxy-mix.jpg
12-push-in-place.jpg
13-place-corner-piece.jpg
14-allow-epoxy-to-cure.jpg
  1. Verify fit with next piece. Immediately after applying the previous piece, if epoxy squeezed out into the next piece space, clean it with the pin tool and alcohol to insure it will not interfere with subsequent pieces proper fit.
  2. Apply epoxy.
  3. Spread epoxy.
  4. Push hard to squeeze out epoxy.
  5. Apply next pieces.
  6. Wait 15-20 minutes before addressing the other side of the platter.

Cementing Chips in Rear of Platter

16-rear-pieces.jpg
15-rear-damage.jpg
17-apply-epoxy-to-surface.jpg
18-place-pieces.jpg
19-wait-for-epoxy-to-cure.jpg
21-small-pieces-thrown-away.jpg
  1. Apply epoxy.
  2. Place pieces.
  3. Wait 1-2 hours before clearing squeezed epoxy.
  4. Small pieces are not used and can be thrown away.

Removing Excess Cured Epoxy

22-bend-a-blade.jpg
23-remove-epoxy-with-blade.jpg
24-ready-for-filler.jpg
  1. Bend blade for better access clearing unwanted cured epoxy. Warning - wear protective eyewear
  2. Let the epoxy cure for 60 or more minutes before removing excess cured epoxy with a blade.
  3. Ready for filler.

What You Will Need - Filling and Sanding for a Seamless Surface

24b-filling-what-needed.jpg

1. Two parts Epoxy filler PC-11 (where to purchase)

2. Dremel with EZ lock sanding disc 120 grit

3. 220 grit sand paper

3. 400 grit sand paper

4. Rag

5. Mini Spatula

6. Paper pad to mix Epoxy on

7. Denatured or 91% Alcohol

IMPORTANT: Ceramic restoration materials are not food safe, liquid or heat proof (over 190 degree F) and repaired items should not be used on cooking or food serving ware more...

Filling Repair Lines and Missing Chips

36-clean-with-alcohol-91.jpg
25-use-filler-epoxy-pc11.jpg
26-push-epoxy-in-cracks.jpg
27-fill-rear-and-wait-cure.jpg
27-wait-for-epoxy-to-cure.jpg
27b-warm-under-lamp.jpg
  1. Wipe all surfaces with a 91% alcohol to remove dust and hand oils prior to applying filler epoxy.
  2. Mix even parts of PC-11 epoxy filler. For ease of application, work in room temperature of 75 degrees F or warmer. We place the PC-11 in a small heater and keep it at 100 degrees F.
  3. Apply thin layer of filler while pushing in to fill cracks and missing fragments.
  4. Allow filler epoxy to cure for 12-24 hours (or longer) at a temperature of 75 degrees F or warmer. We place our filled projects in a 140 degrees F oven over night.
  5. Placing under a lamp is another good option to optimize hardness for better sanding performance. Place at least 12" away from repair item to avoid overheating.

Sanding Cured Filler Using Dremel

28-sand-with-dremel-ez-disc.jpg
29-low-speed-light-pressure.jpg
30-sand-rim.jpg
31-roud-one-sanding.jpg
32-repeat-sanding-in-rear.jpg
33-blow-dust-away.jpg
  1. Use Dremel EZ lock sanding disc 120 grit for sanding.
  2. Use low speed to avoid burn marks and apply light pressure. Leave the last 10% or so for sanding by hand.
    Warning - wear protective eyewear.
  3. If Dremel is not available, sanding the whole job by hand (using grit 220 sandpaper) will take longer but will yield the same results.
  4. Repeat process on platter's other side.
  5. Blow or wipe dust away.

Second Sanding Phase

34-sand-by-hand-grit-220.jpg
35-sand-light-pressure.jpg
37-wipe-thoroughly.jpg
  1. Continue sanding by hand using grit 220.
  2. Apply long strokes for accurate surface continuity If upon inspection, missed cracks are found, repeat the steps above for the selected areas.
  3. Use 91% alcohol for clean up

Fine Filling

38-use-fine-spachelor-tool.jpg
39-use-pc-11-feeler.jpg
40-even-parts-filler-epoxy.jpg
41-inspect-for-pits-cracks-.jpg
42-fill-pits-and-defects.jpg
43-wait-till-cured.jpg
  1. After the first round of sanding, second finer filling is required using a small sepulcher tool.
  2. Same filler (PC-11) is used for second application.
  3. Mix well the epoxy filler two even parts.
  4. For seamless surface fill the defects with PC-11 lightly.
  5. Wait for filler second layer to cure in a warm room (see more above) before sanding

Fine Sanding and Polishing

44-sand-with-220-and-400-gr.jpg
45-wipe-with-alcohol.jpg
  1. Sand second layer by hand with long strokes using grit 220, then grit 400 and finish with grit 3600 (where to purchase). It may be necessary to apply a third or forth layer if UV / light close inspection reveals more surface defects.
  2. Wipe with alcohol for better paint bond

Painting

46-mix-background-color.jpg
47-air-brush-background.jpg
48-airbrush-glaze-layer.jpg
49-mix-colors-acrylic.jpg
50-fill-in-details.jpg
51-paint-acrylic.jpg
52-coloring-details.jpg
  1. Mix acrylic paints to match background off-white color.
  2. Airbrush over the repair line and taper off for smooth color integration to original background glaze.
  3. Painting over the repair line will erase painting details which will be replenished later.
  4. Wait a day or two for the acrylic paint to dry well and apply thin layer of cold glaze to protect the applied the painted areas.
  5. Mix acrylic paints to match to missing colors details.
  6. Use fine brushes to apply colors.
  7. For translucent effect, paint several coats of thinned paints.
  8. In this example, apply black color last.

Painting theory tutorial - seamless colors

Glazing

53-apply-cold-glaze.jpg
54-platter-glazed.jpg
55-ready-for-shipment.jpg
  1. Wait for painting to properly dry (a couple of days) and airbrush clear glaze.
  2. Second layer of clear glaze may be required. Sand surface with a 3200 grit micro-mesh (after waiting a day or two for 1st layer curing), wipe dust off and reapply cold glaze.
  3. Platter ready for shipment.

KINTSUGI ART - Repairing Pottery With Gold | How Is It Made: 22 Minutes Video

What is Kintsugi? How is Kintsugi Made?  Kintsukuroi Making Lesson and Metaphor

More Ceramic and Sculpture Repair Lessons

small-porcelain-hand.jpg
foot-sculpting.jpg
sculpture-repair-missing-piece-made-of-clay.jpg
metal-work.jpg

See Step by Step Video Showing Pottery Repair

How to repair broken ceramic and pottery